Table 1 Feed ratios of synthesized poly (LVCS-g-PNIPAAm) gels (n = 3)

From: Fabrication and evaluation of smart pH/thermo dual-responsive injectable intratumoral in situ depot hydrogels for controlled 5-FU delivery

Codes

PNIPAAm (g)

LVCS (g)

APS (g)

GA (g)

Tsol–gel (°C)

Gelation time (GT)

H2O (g)

IP-1

0.500

37

No gelation

10 g

IP-2

1

0.020

34 ± 0.21

 17 min

10 g

IP-3

1.5

0.020

34 ± 0.20

 10 min

10 g

IPLVCS-1

1

0.150

0.015

0.015

35 ± 0.23

 8 min

10 g

IPLVCS-2

1

0.200

0.015

0.015

35 ± 0.27

 10 min

10 g

IPLVCS-3

1.5

0.200

0.015

0.015

34 ± 0.90

 07 min

10 g

IPLVCS -4

2.0

0.200

0.015

0.015

33 ± 0.20

 06 min

10 g

IPLVCS -5

2.5

0.200

0.015

0.020

34 ± 0.05

 04 min

10 g

IPLVCS -6

2.5

0.200

0.015

0.025

33 ± 0.60

 02 min

10 g